性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | |
比重 | ASTMD792 | 1.04 | g/cm3 | |
密度 | ISO1183 | 1.04 | g/cm3 | |
弹性体 | TestMethod | NominalValue | Unit | |
伸长率-横向流量(断裂,23°C) | ASTMD412 | 600 | % | |
伸长率-横向流量(断裂,23°C) | ISO37 | 600 | % | |
CompressionSet2(125°C,70hr) | ASTMD395B | 55 | % | |
CompressionSet3(125°C,70hr) | ISO815 | 55 | % | |
肖氏硬度(邵氏A,15秒,23°C) | ISO868 | 53 | ||
空气中拉伸强度的变化率 | 100°C,168hr | ASTMD573 | -28 | % |
空气中拉伸强度的变化率 | 125°C,168hr | ASTMD573 | -61 | % |
空气中拉伸强度的变化率 | 100°C,168hr | ISO188 | -28 | % |
空气中拉伸强度的变化率 | 125°C,168hr | ISO188 | -61 | % |
空气中极限伸长率的变化率 | 100°C,168hr | ASTMD573 | -14 | % |
空气中极限伸长率的变化率 | 125°C,168hr | ASTMD573 | -70 | % |
在空气中断裂时拉伸应力变化 | 100°C,168hr | ISO188 | -14 | % |
在空气中断裂时拉伸应力变化 | 125°C,168hr | ISO188 | -70 | % |
空气中硬度计硬度的变化率 | ShoreA,100°C,168hr | ASTMD573 | -4.0 | |
空气中硬度计硬度的变化率 | 邵氏A,125°C,168hr | ASTMD573 | 8.0 | |
空气中邵氏硬度的变化率 | ShoreA,100°C,168hr | ISO188 | -4.0 | |
空气中邵氏硬度的变化率 | 邵氏A,125°C,168hr | ISO188 | 8.0 | |
拉伸强度的变化率 | 23°C,168hr,inEthanol,95% | ASTMD471 | -17 | % |
拉伸强度的变化率 | 23°C,168hr,inHydrochloricAcid,10% | ASTMD471 | -1.0 | % |
拉伸强度的变化率 | 23°C,168hr,inIRM903Oil | ASTMD471 | -85 | % |
拉伸强度的变化率 | 23°C,168hr,inSodiumHydroxide,50% | ASTMD471 | 1.0 | % |
拉伸强度的变化率 | 23°C,168hr,在水中 | ASTMD471 | 2.0 | % |
拉伸强度的变化率 | 23°C,168hr,inEthanol,95% | ISO1817 | -17 | % |
拉伸强度的变化率 | 23°C,168hr,inHydrochloricAcid,10% | ISO1817 | -1.0 | % |
拉伸强度的变化率 | 23°C,168hr,inIRM903Oil | ISO1817 | -85 | % |
拉伸强度的变化率 | 23°C,168hr,inSodiumHydroxide,50% | ISO1817 | 1.0 | % |
拉伸强度的变化率 | 23°C,168hr,在水中 | ISO1817 | 2.0 | % |
极限伸长率的变化率 | 23°C,168hr,inEthanol,95% | ASTMD471 | -3.0 | % |
极限伸长率的变化率 | 23°C,168hr,inHydrochloricAcid,10% | ASTMD471 | -9.0 | % |
极限伸长率的变化率 | 23°C,168hr,inIRM903Oil | ASTMD471 | -68 | % |
极限伸长率的变化率 | 23°C,168hr,inSodiumHydroxide,50% | ASTMD471 | -7.0 | % |
极限伸长率的变化率 | 23°C,168hr,在水中 | ASTMD471 | -12 | % |
断裂时拉伸应力变化 | 23°C,168hr,inEthanol,95% | ISO1817 | -3.0 | % |
断裂时拉伸应力变化 | 23°C,168hr,inHydrochloricAcid,10% | ISO1817 | -9.0 | % |
断裂时拉伸应力变化 | 23°C,168hr,inIRM903Oil | ISO1817 | -68 | % |
断裂时拉伸应力变化 | 23°C,168hr,inSodiumHydroxide,50% | ISO1817 | -7.0 | % |
断裂时拉伸应力变化 | 23°C,168hr,在水中 | ISO1817 | -12 | % |
硬度计硬度的变化率2 | ShoreA,23°C,168hr,inEthanol,95% | ASTMD471 | 2.0 | |
硬度计硬度的变化率2 | ShoreA,23°C,168hr,inHydrochloricAcid,10% | ASTMD471 | 4.0 | |
硬度计硬度的变化率2 | ShoreA,23°C,168hr,inIRM903Oil | ASTMD471 | -33 | |
硬度计硬度的变化率2 | ShoreA,23°C,168hr,inSodiumHydroxide,50% | ASTMD471 | 4.0 | |
硬度计硬度的变化率2 | ShoreA,23°C,168hr,inWater | ASTMD471 | 5.0 | |
ChangeinShoreHardness | ShoreA,23°C,168hr,inEthanol,95% | ISO1817 | 2.0 | |
ChangeinShoreHardness | ShoreA,23°C,168hr,inHydrochloricAcid,10% | ISO1817 | 4.0 | |
ChangeinShoreHardness | ShoreA,23°C,168hr,inIRM903Oil | ISO1817 | -33 | |
ChangeinShoreHardness | ShoreA,23°C,168hr,inSodiumHydroxide,50% | ISO1817 | 4.0 | |
ChangeinShoreHardness | ShoreA,23°C,168hr,inWater | ISO1817 | 5.0 | |
UL阻燃等级 | 1.1mm | UL94 | HB | |
UL阻燃等级 | 2.9mm | UL94 | HB |
TPV 8211-55B100塑料供应商,长期销售美国埃克森美孚化工生产的TPV原料,以上是“TPV Santoprene™ 8211-55B100”塑胶料的物性表参数.近期代理商可转仓交易:美国RTP PP RTP 154 LF 阻燃性,流动性低,注射成型
中国成都晨光博达 氟橡胶 Boda BDF-KK2802
台湾南帝化学 TPE Dynaprene® VER8500 注射成型
美国Buckeye Polymers TPV BP Flex 7500 VPL BLK
美国路博润 TPU聚醚 Pearlthane® 16N95UV
德国凯柏胶宝 TPE COPEC® CC6OCZ (Series: VS/AD1)
英国ELASTO TPE Dryflex® 4092
美国利安德巴塞尔 TPO Supol HR570E 填料,矿物填料.汽车领域的应用,汽车外部零件
美国普立万 TPE Dynaflex™ G2755-1000-00 耐臭氧性能,可回收材料,抗紫外线性能良好,注射成型,挤出 消费品应用领域,个人护理,包覆成型,通用,柔软的把手,透明或半透明配件,柔软触感应用
美国埃克森美孚化工 EVA Escorene™ Ultra LD 708.62
意大利Guarniflon PTFE Flontech® FT-CARR25-3 填料,碳纤维增强材料,25%填料按重量.
德国开德阜 PPA AKROMID® T1 GF 50 natural (3376)
美国RTP PPA RTP 4082 AR 15 填料,碳纤维增强材料,15%填料按重量,芳族聚酰胺纤维,15%填料按重量.
● TPV 埃克森美孚 103-50 其它
● TPV 美国埃克森美孚 201-64
良好的抗蠕变性,耐臭氧性能,绝缘,可回收材料,良好的耐热老化性能,良好的着色性,良好的电气性能,尺寸稳定性良好,低的压缩变形性,耐疲劳性能,耐化学性良好,片材挤出成型,共挤出成型,注吹成型,吹塑成型,挤出,注射成型,挤出吹塑成型,多次注射成型,型材挤出成型
● TPV 三井化学 G800BS
注塑
● TPV 日本三菱 Trexprene A64BW-HF
● TPV 美国RTP RTP 2800 B-75A HB
注射成型