玻纤增强 其它 注塑 | |
一般用途 | |
特性:玻纤增强30% |
性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | |
吸水率 | 23℃ | ASTM D-570 | 无水|0.6 | % |
吸水率 | 23℃ | ASTM D-570 | 1.5%水|- | % |
比重 | ASTM D-792 | 无水|1.37 | ||
比重 | ASTM D-792 | 1.5%水|- | ||
泰伯磨耗量 | (1000g,CS-17)23℃ | ASTM D-1044 | 无水|24 | mg/1000次 |
泰伯磨耗量 | (1000g,CS-17)23℃ | ASTM D-1044 | 24|- | mg/1000次 |
压缩强度 | 23℃ | ASTM D-695 | 无水|1850 | Kg/cm2 |
压缩强度 | 23℃ | ASTM D-695 | 1.5%水|- | Kg/cm2 |
IZOD冲击强度 | -40℃ | 无水|60 | kgcm/cm2 | |
IZOD冲击强度 | -40℃ | 1.5%水|70 | kgcm/cm2 | |
洛氏硬度 | 23℃ | ASTM D-785 | 无水|121 | R-标度 |
洛氏硬度 | 23℃ | ASTM D-785 | 1.5%水|- | R-标度 |
断裂伸长率 | -40℃ | ASTM D-638 | 无水|3.5 | % |
断裂伸长率 | -40℃ | ASTM D-638 | 1.5%水|- | % |
断裂伸长率 | 80℃ | ASTM D-638 | 无水|8.5 | % |
断裂伸长率 | 80℃ | ASTM D-638 | 1.5%水|- | % |
挠曲模量 | -40℃ | ASTM D-790 | 无水|85000 | Kg/cm2 |
挠曲模量 | -40℃ | ASTM D-790 | 1.5%水|60000 | Kg/cm2 |
抗剪强度 | 23℃ | ASTM D-732 | 无水|970 | Kg/cm2 |
抗剪强度 | 23℃ | ASTM D-732 | 1.5%水|830 | Kg/cm2 |
抗拉屈服强度 | 80℃ | ASTM D-638 | 无水|1100 | Kg/cm2 |
抗拉屈服强度 | 80℃ | ASTM D-638 | 1.5%水|900 | Kg/cm2 |
抗拉屈服强度 | -40℃ | ASTM D-638 | 无水|2350 | Kg/cm2 |
抗拉屈服强度 | -40℃ | ASTM D-638 | 1.5%水|2100 | Kg/cm2 |
洛氏硬度 | 23℃ | ASTM D-785 | 无水|97 | M-标度 |
洛氏硬度 | 23℃ | ASTM D-785 | 1.5%水|- | M-标度 |
挠曲强度 | 80℃ | ASTM D-790 | 无水|1750 | Kg/cm2 |
挠曲强度 | 80℃ | ASTM D-790 | 1.5%水|1250 | Kg/cm2 |
挠曲强度 | -40℃ | ASTM D-790 | 无水|3000 | Kg/cm2 |
挠曲强度 | -40℃ | ASTM D-790 | 1.5%水|3000 | Kg/cm2 |
挠曲模量 | 80℃ | ASTM D-790 | 无水|50000 | Kg/cm2 |
挠曲模量 | 80℃ | ASTM D-790 | 1.5%水|40000 | Kg/cm2 |
IZOD冲击强度 | -40℃,V缺口1/2 | ASTM D-256 | 无水|8 | kgcm/cm |
IZOD冲击强度 | -40℃,V缺口1/2 | ASTM D-256 | 1.5%水|10 | kgcm/cm |
压缩强度 | -40℃ | ASTM D-695 | 无水|2600 | Kg/cm2 |
压缩强度 | -40℃ | ASTM D-695 | 1.5%水|- | Kg/cm2 |
IZOD冲击强度 | 23℃,无缺口1/8 | 无水|65 | kgcm/cm2 | |
IZOD冲击强度 | 23℃,无缺口1/8 | 1.5%水|78 | kgcm/cm | |
断裂伸长率 | 23℃ | ASTM D-638 | 无水|5 | % |
断裂伸长率 | 23℃ | ASTM D-638 | 1.5%水|5 | % |
挠曲强度 | 23℃ | ASTM D-790 | 无水|2600 | Kg/cm2 |
挠曲强度 | 23℃ | ASTM D-790 | 1.5%水|1900 | Kg/cm2 |
抗剪强度 | 80℃ | ASTM D-732 | 无水|760 | Kg/cm2 |
抗剪强度 | 80℃ | ASTM D-732 | 1.5%水|- | Kg/cm2 |
IZOD冲击强度 | 23℃,V-缺口1/2 | ASTM D-256 | 无水|9 | kgcm/cm |
IZOD冲击强度 | 23℃,V-缺口1/2 | ASTM D-256 | 1.5%水|14 | kgcm/cm |
压缩强度 | 80℃ | ASTM D-695 | 无水|1100 | Kg/cm2 |
压缩强度 | 80℃ | ASTM D-695 | 1.5%水|- | Kg/cm2 |
抗拉屈服强度 | 23℃ | ASTM D-638 | 无水|1800 | Kg/cm2 |
抗拉屈服强度 | 23℃ | ASTM D-638 | 1.5%水|1350 | Kg/cm2 |
抗电弧性 | 1/8 | ASTM D-495 | 无水|114 | s |
抗电弧性 | 1/8 | ASTM D-495 | 1.5%水|120 | s |
损耗因数 | 103Hz | ASTM D-150 | 无水|0.02 | |
损耗因数 | 103Hz | ASTM D-150 | 1.5%水|0.08 | |
介电常数 | 106Hz | ASTM D-150 | 无水|3.9 | |
介电常数 | 106Hz | ASTM D-150 | 1.5%水|4.0 | |
介电强度 | 1/8 | ASTM D-149 | 无水|20 | KV/mm |
介电强度 | 1/8 | ASTM D-149 | 1.5%水|17 | KV/mm |
PA66 CM3001G-30塑料供应商,长期销售日本东丽生产的PA66原料,以上是“PA66 CM3001G-30”塑胶料的物性表参数.近期代理商可转仓交易:海湾石油 PP 6T208 均聚,含20%滑石填充增强
德国巴斯夫 POM N2720M43 其它
日本三菱 HDPE HF210A 薄膜 牵伸带,胶带等
三菱石化 PP PY230 挤出 单丝,牵伸带等
三井东压 PP JH-SA20 聚烯烃复合树脂 耐热,高刚性制品
杰达塑化 PPS TR3 其它
宁波福天 PA6 A212 20%玻纤增强 可用于线圈骨架,滑轮,电动工具壳体
美国英力士 PP H03W-00 拉丝
美国陶氏 LLDPE DNDB-7441 NT 7 产品商标DOW 挤出级用
台塑美国 LLDPE L63550U4 产品商标,Formolene 玩具,农业和化工储罐等
雪佛龙菲利普斯 PP HMV-035 均聚,纤维级,抗紫外线 绳索,室外地毯
利安德巴塞尔 PP BR33GC 传统的熔体流动尺寸稳定性良好耐冲击性高刚度高抵抗紫外辐射良好 汽车内饰部分
北欧化工 HDPE VL4580 其它 适合针织和梭织面料
利安德巴塞尔 PP 4323 其它 汽车应用
● PA66 美国RTP 282H
玻纤增强,注塑
● PA66 韩国LG化学 Lumid GP2200B(W)
填料:玻璃纤维增强材料, 20% 填料按重量。
● PA66 美国RTP 200.5 FR
注塑
● PA66 韩国可隆 KN333G25
玻璃纤维增强材料
● PA66 美国RTP 283 FR HS
碳纤增强