| 性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | |
| 比重 | ASTMD792 | 1.11 | g/cm3 | |
| 密度 | ISO1183 | 1.11 | g/cm3 | |
| 熔流率(熔体流动速率) | 280°C/5.0kg | ASTMD1238 | 18 | g/10min |
| 熔流率(熔体流动速率) | 300°C/5.0kg | ASTMD1238 | 43 | g/10min |
| 溶化体积流率(MVR) | 280°C/5.0kg | ISO1133 | 17.6 | cm3/10min |
| 溶化体积流率(MVR) | 300°C/5.0kg | ISO1133 | 41.0 | cm3/10min |
| 收缩率-流动(3.20mm) | InternalMethod | 0.50to0.80 | % | |
| 吸水率(饱和,23°C) | ISO62 | 0.27 | % | |
| 吸水率(平衡,23°C,50%RH) | ISO62 | 0.045 | % | |
| 拉伸模量2 | ASTMD638 | 2450 | MPa | |
| 拉伸模量 | ISO527-2/1 | 2430 | MPa | |
| 抗张强度3(屈服) | ASTMD638 | 56.2 | MPa | |
| 拉伸应力(屈服) | ISO527-2/50 | 54.0 | MPa | |
| 抗张强度3(断裂) | ASTMD638 | 46.8 | MPa | |
| 拉伸应力(断裂) | ISO527-2/50 | 47.8 | MPa | |
| 伸长率3(屈服) | ASTMD638 | 4.3 | % | |
| 拉伸应变(屈服) | ISO527-2/50 | 4.0 | % | |
| 伸长率4(断裂) | ASTMD638 | 28 | % | |
| 拉伸应变 | 断裂 | ISO527-2 | 28 | % |
| 拉伸应变 | 断裂 | ISO527-2/50 | 28 | % |
| 弯曲模量4(50.0mm跨距) | ASTMD790 | 2400 | MPa | |
| 弯曲模量5 | ISO178 | 2390 | MPa | |
| FlexuralStress5,6 | ISO178 | 90.0 | MPa | |
| 弯曲强度4(屈服,50.0mm跨距) | ASTMD790 | 90.0 | MPa | |
| 简支梁缺口冲击强度7(23°C) | ISO179/1eA | 19 | kJ/m2 | |
| 悬壁梁缺口冲击强度 | -30°C | ASTMD256 | 120 | J/m |
| 悬壁梁缺口冲击强度 | 23°C | ASTMD256 | 200 | J/m |
| 悬壁梁缺口冲击强度8 | -30°C | ISO180/1A | 11 | kJ/m2 |
| 悬壁梁缺口冲击强度8 | 23°C | ISO180/1A | 16 | kJ/m2 |
| 装有测量仪表的落镖冲击(23°C,TotalEnergy) | ASTMD3763 | 46.0 | J | |
| 载荷下热变形温度 | 1.8MPa,未退火,3.20mm | ASTMD648 | 106 | °C |
| 载荷下热变形温度 | 1.8MPa,未退火,6.40mm | ASTMD648 | 113 | °C |
| HeatDeflectionTemperature9(1.8MPa,Unannealed,64.0mmSpan) | ISO75-2/Af | 107 | °C | |
| 维卡软化温度 | ASTMD152510 | 127 | °C | |
| 维卡软化温度 | —— | ISO306/B50 | 127 | °C |
| 维卡软化温度 | —— | ISO306/B120 | 129 | °C |
| 线形热膨胀系数-流动(-40到40°C) | ASTME831 | 8.4E-5 | cm/cm/°C | |
| 线形热膨胀系数-流动(-40到40°C) | ISO11359-2 | 8.4E-5 | cm/cm/°C | |
| 线形热膨胀系数-横向(-40到40°C) | ASTME831 | 8.5E-5 | cm/cm/°C | |
| 线形热膨胀系数-横向(-40到40°C) | ISO11359-2 | 8.5E-5 | cm/cm/°C | |
| DraegerTubeToxicity11 | Flaming:1.52mm | Pass | ||
| DraegerTubeToxicity11 | Non-Flaming:1.52mm | Pass | ||
| FlameSpreadIndex(1.52mm) | ASTME162 | 15.0 | ||
| NBSSmokeDensity | Flaming,20min:3.20mm | ASTME662 | 126 | |
| NBSSmokeDensity | Flaming,4min:1.52mm | ASTME662 | 29.0 | |
| NBSSmokeDensity | Flaming,4min:3.20mm | ASTME662 | 35.0 | |
| NBSSmokeDensity | Non-Flaming,4min:1.52mm | ASTME662 | 7.00 | |
| VerticalBurnTest | Testa(60s,1.52mm),passesat | FAR25.853 | 0.0 | hr |
| VerticalBurnTest | Testb(12s,1.52mm),passesat | FAR25.853 | 4.00 | sec |
PPO(PPE) NH4030B resin塑料供应商,长期销售沙伯基础生产的PPO(PPE)原料,以上是“PPO(PPE) NORYL™ NH4030B resin”塑胶料的物性表参数.近期代理商可转仓交易:土耳其Elastron TPV Elastron® V V101.D51.N 良好的着色性,可粘结性,硬度高,耐化学性良好,注射成型,挤出
中国苏州奥斯汀 TPU聚脂 Texalan® 3 Series 372D 高拉伸强度良好,耐磨损性,耐油性能,高弹性,耐低温,抗撞击性高,吹塑成型,注射成型,压延,薄膜挤出,挤出,共挤出成型
中国深圳盛嘉伦 TPE Gallonprene® GP550-7503 优良外观,高弹性,无卤,抗微生物,可焊接,挤出,型材挤出成型 型材,密封件
美国Teknor Apex TPE Sarlink® TPE EE-1290N NAT 高密度,挤出 汽车领域的应用,汽车外部装饰,通用,汽车外部零件
韩国现代 TPE Plasmer 1040DN/1002 可回收材料 汽车领域的应用
日本旭化成弹性体 SEBS Tuftec™ M1943
中国上海林艮 PP+EPDM Deprene 101-80 良好的柔韧性,通用,耐化学性良好,注射成型,挤出 密封件,电线电缆应用,管道,通用
美国Polymer Dynamix EVA EverGlide® MB3950
美国RTP PPS RTP 1311 填料,玻璃纤维增强材料,60%填料按重量.
美国Polymer Dynamix PPA DynaMix™ 4100-28CF 填料,碳纤维增强材料.汽车领域的应用,航空航天应用,军事应用,工业应用
沙伯基础 PEI ULTEM™ 4211 resin 填料,玻璃纤维增强材料,20%填料按重量.
意大利Soredi POM共聚 Niform 130 共聚物,注射成型 通用
德国POLYMA POM均聚 POLYFORM C 9 natural
美国PTS PC TRISTAR® PC-10FRNH 无溴,脱模性能良好,无氯,阻燃性
美国RTP PC RTP 399 X 95997 B 导热,导电,注射成型